H68 Brass Tube: Copper Content, Condenser Service and Brazing Guide
H68 brass tube is a high-copper, single-phase copper-zinc tube used where a part must carry water, steam condensate or a non-aggressive process fluid and still be bent, expanded or brazed into an assembly. The grade is close to the top of the ordinary brass range, so it is more ductile and more corrosion-resistant than H62, but it is not a dezincification-resistant alloy and it is not a substitute for copper-nickel in seawater.
What H68 Brass Tube Is and Where It Is Used
H68 is a wrought brass with a nominal copper content of 67–70% and zinc making up almost all of the remainder. At that composition the microstructure is essentially single-phase alpha brass at room temperature. The alpha phase is soft and ductile, which is why H68 can be cold drawn into thin-wall tube, bent through tight radii and expanded into a tube sheet without cracking. The same structure is the reason the tube solders and brazes more easily than the duplex H59 grades.
The largest use is heat-transfer tubing. H68 tube appears in shell-and-tube heat exchangers, condensers, radiateurs, oil coolers, refrigeration condensers and low-pressure steam traps. It is also used in water supply lines, sanitary fittings, decorative furniture tube, musical instrument tubing and small pneumatic or hydraulic return lines where the pressure is modest and the fluid is not aggressive.
The grade is popular because it occupies a useful middle ground. H62 is cheaper and stronger but less ductile and less resistant to dezincification. Cuivre, C12200, is more conductive and more corrosion-resistant but costs much more and is softer. H68 gives a fabricator a tube that bends well, brazes well and resists ordinary tap water and condensed moisture, at a cost below copper.
H68 tube should not be specified for seawater, chlorinated pool water, strong acids or ammonia. In those environments dezincification and stress-corrosion cracking are real risks. A copper-nickel grade, a DZR brass or a proven polymer lining is the correct choice. The fact that the tube is “brass” does not make it suitable for every water service.

Désignation de qualité et composition chimique
H68 is specified in China by GB/T 5231 and corresponds broadly to the ISO CuZn33 family. The high copper level is deliberate: it keeps the alloy single-phase, improves cold ductility and raises resistance to general corrosion. The table shows a typical wrought-tube window. Exact limits depend on the standard edition and on the mill’s own grade control, so the certificate should always be read against the purchase specification.
| Élément | Typical H68 range (%) | Rôle dans l'alliage | Purchasing note |
|---|---|---|---|
| Cu | 67.0–70.0 | Alpha-phase stabiliser; résistance à la corrosion | Ci-dessous 67% raises beta fraction and reduces ductility |
| Zn | Équilibre | Strength and cost control | Zinc loss in melting is normal; verify by analysis |
| Pb | ≤ 0.05 | Residual impurity | Keep low for potable water and brazing |
| Fe | ≤ 0.10 | Grain control | Excess iron forms hard inclusions |
| Sn | ≤ 0.10 | Minor strength | Residual; not a substitute for tin bronze |
| Al | ≤ 0.05 | Résiduel de désoxydation | Too much aluminium hurts hot workability |
| Sb | ≤ 0.005 | Unintended impurity | Brittle phase above limit |
| Bi | ≤ 0.002 | Unintended impurity | Hot-short cracking in drawing |
| P. | ≤ 0.01 | Residual deoxidiser | Excess phosphorus embrittles the tube |
| Impuretés totales | ≤ 0.5 | Scrap control | Spectrography is the practical check |
Typical GB/T 5231 window for H68 wrought brass tube. Confirm lead limits separately for potable-water or food-contact service.
The copper range is narrow for a reason. A heat exchanger tube is expanded into a tube sheet and then subjected to thermal cycling; if the copper falls below the specified minimum, the tube becomes stronger but less ductile, and the expansion can crack the tube end. At the top of the range the tube is softer and easier to expand, but it is also easier to damage during handling. The mill’s analysis and the fabricator’s expansion procedure must be matched.
Propriétés mécaniques
H68 tube is normally supplied annealed, designated O or O60, because the cold-drawing operation leaves the tube too hard for expansion and bending. A stress-relieved temper is available for parts that need straighter tube or better dimensional stability. The table gives typical room-temperature values for annealed thin-wall tube; the actual values depend on wall thickness, drawing reduction and the final anneal.
| Propriété | Recuit (O60) | Stress relieved | Étiré à froid (dur) |
|---|---|---|---|
| 0.2% contrainte de preuve, Rp0.2 (MPa) | 90–170 | 150–230 | 260–360 |
| Résistance à la traction, Chambre (MPa) | 300–400 | 360–450 | 480–620 |
| Élongation, UN (%) | 35–50 | 25–35 | 8–18 |
| Dureté, HT | 65–90 | 90–115 | 120–160 |
| Conductivité électrique (% SIGC) | 22–26 | 22–26 | 21–25 |
| Conductivité thermique (W/m·K) | 85–105 | 85–105 | 80–100 |
Typical room-temperature values for annealed H68 tube. Thin-wall tube is usually tested in the longitudinal direction; confirm sampling and test method on the mill report.
The practical message is that temper controls the fabrication route. An annealed tube can be bent to a tight radius and rolled into a tube sheet. A hard-drawn tube is stronger but will spring back and may crack at the bend. If a drawing calls for H68 without a temper, the fabricator may receive a tube that is technically correct but impossible to expand without annealing.

Dimensions, Tolerances and Supply Forms
H68 tube is ordered by outside diameter, épaisseur de paroi, temper and length. The wall is the critical dimension for pressure service, but the outside diameter controls the fit in the tube sheet or fitting. A tube that is at the high limit of the OD tolerance may not enter a close-fit hole; a tube at the low limit may leak after expansion. Both dimensions should be specified with the intended joining method in mind.
| Fonctionnalité | Gamme commune | Tolérance typique | Ordering note |
|---|---|---|---|
| Diamètre extérieur | 4–60 mm | ±0.05 mm or ±0.5% | State the fit: expansion, brazing or compression |
| Épaisseur de paroi | 0.5–4.0 mm | ±10% or ±0.05 mm | Minimum wall is the pressure-safety number |
| Longueur | 0.5–6 m | +5 / 0 mm | Straight lengths or coiled pancake |
| Rectitude | — | 1–3 mm per metre | Critical for tube-sheet assembly |
| Ovalité | — | ≤ 80% of OD tolerance | Affects expansion and sealing |
| Eccentric wall | — | ≤ 10% of nominal wall | Thin side is the first to fail |
| Surface | — | Brillant, pickled or annealed | Pickled tube needs a clean rinse |
| Se termine | — | Coupe à la scie, ébavuré, plafonné | Caps prevent chips entering the bore |
Typical commercial windows for drawn H68 tube. Pressure service requires a hydrostatic or eddy-current test in addition to dimensional inspection.
Two tolerances deserve extra attention. Eccentric wall, sometimes called wall offset, means the bore is not concentric with the outside diameter. A tube with a nominal 1.5 mm wall and 12% eccentricity has a thin side of about 1.32 mm, which may be below the design minimum even though the average wall is correct. Ovality matters for expansion: an oval tube does not seal evenly in a tube sheet and can leak on the first thermal cycle.
Supply form is another decision. Straight lengths are used for heat exchangers and for automatic brazing; pancake coils are used for plumbing and refrigeration. A coil has a residual curvature that must be straightened before close-tolerance machining, and the coil diameter affects the minimum bend radius the tube can accept. If the tube will be bent in a press or on a CNC bender, order annealed straight lengths and state the bend radius on the drawing.
How H68 Tube Is Made
The process starts with a cast billet or extrusion billet prepared from cathode copper and zinc. The melt is covered to limit zinc loss, deoxidised with a small phosphorus addition, and analysed before casting. The billet is homogenised and then extruded into a hollow shell or a solid rod, depending on the mill route. For tube, the shell is cold drawn over a mandrel or pilgered to reduce wall thickness and improve concentricity.
Cold drawing is done in several passes with interpass annealing. Each pass reduces the wall and raises strength; the anneal restores ductility and recrystallises the grain. The final anneal is usually a bright anneal in a reducing atmosphere or a controlled-atmosphere furnace, followed by a clean rinse. If the anneal is too cold, the tube remains hard and springs back during bending; if it is too hot, the grain coarsens and the tube loses strength and surface quality.
Après recuit, the tube is straightened, couper, deburred and inspected. Heat-exchanger tube is normally eddy-current tested to detect longitudinal defects, and pressure tube is hydrostatically tested. The tests are not interchangeable: eddy current finds seams and cracks, while a hydrostatic test proves that the wall can hold pressure. A purchase order for condenser tube should name both tests, the test pressure and the acceptance standard.
The defects that most often cause field failures are eccentric wall, longitudinal seams, residual drawing lubricant and inadequate annealing. Eccentric wall comes from a worn mandrel or a misaligned draw bench. Seams come from a defective billet or a folded oxide layer. Residual lubricant is a cleaning problem and will contaminate brazing flux or drinking water. Inadequate annealing shows up as cracking at the tube-sheet expansion or as a bend that will not hold its radius.
Pliant, Expansion and Brazing
H68 tube bends well in the annealed condition. For a 90-degree bend, a centreline radius of about 2 à 3 times the outside diameter is practical for thin-wall tube; tighter radii need a mandrel, a slower bend and sometimes a local anneal. Do not bend a hard-drawn tube without annealing. Springback is proportional to yield strength, so a hard tube will not hold the intended angle and may crack on the outside of the bend.
Tube-sheet expansion is a controlled plastic deformation. The tube is rolled with a mandrel that expands the wall into the sheet hole, creating a seal and a light interference fit. The expansion should be uniform along the sheet thickness; over-rolling work-hardens the tube end and can cause stress-corrosion cracking later. Under-rolling leaves a leak path. The correct roll diameter, torque and lubrication should come from a procedure qualification, not from a generic chart.
Brazing is the usual joining method for H68. Use a silver-based filler and a fluoride flux, heat the joint evenly and keep the flame moving. H68 has a narrow hot-short range: overheating causes zinc loss, grain coarsening and a porous joint that will leak. After brazing, remove the flux residue with warm water and a brush; residual flux is hygroscopic and will corrode the tube in storage. Pour l'eau potable, use a lead-free filler and a flux that is approved for the application.
Soldering is possible for low-pressure water and decorative work, but lead-containing solders should not be used on potable-water lines. Tin-antimony or tin-copper lead-free solders are the correct choice. The joint gap, cleanliness and heat input matter more than the solder brand; a poorly fitted joint with a large gap will not fill by capillary action, no matter how much solder is applied.
Selection Rules for Buyers
- Choose H68 for annealed heat-transfer tube and general water service. Its single-phase structure bends and expands well.
- Choose H62 when cost dominates and the tube will not be severely bent. H62 is stronger but less ductile and less resistant.
- Choose copper C12200 for potable water and high-conductivity heat transfer. It is more resistant and more conductive, at a higher price.
- Choose copper-nickel for seawater and chloride-rich cooling water. H68 is not a marine alloy.
- Do not choose H68 for chlorinated pool water or ammonia. Dezincification and stress-corrosion cracking are likely.
- Spécifier l'humeur, test method and minimum wall. A grade alone does not define a pressure-safe tube.
The selection should also consider the joining method. If the tube will be expanded into a tube sheet, annealed tube with a tight OD tolerance and low eccentricity is required. If the tube will be brazed into a manifold, a clean, dry bore and a consistent wall are more important than a tight OD. If the tube will be bent on a CNC bender, specify the bend radius and the permissible ovality after bending, not only the as-supplied dimensions.
Wall thickness is a pressure decision, not a stiffness decision. A thicker wall raises burst pressure and crush resistance, but it also raises bending force, reduces heat-transfer area and increases weight and cost. For a heat exchanger, the thermal design usually sets the wall; for a water line, the pressure rating and the corrosion allowance set it. Do not add wall “for safety” without checking the expansion procedure and the pressure drop.
Installation and Service Rules
Support H68 tube at intervals that prevent sag and vibration. A long horizontal run that is supported only at the ends will sag in service, trap water and flex at the joints. Use saddle supports with a compatible liner; direct contact with steel in a wet environment creates a galvanic couple that attacks the steel and can accelerate brass corrosion. Keep the tube away from direct contact with lead, copper and stainless steel where condensate can bridge the joint.
Allow for thermal expansion. H68 expands at roughly 0.017–0.019% per °C, donc un 10 m run heated from 20 °C to 80 °C grows by about 10 mm. If the run is rigidly anchored at both ends, that growth becomes a compressive load on the tube and the fittings. Use flexible couplings, expansion loops or sliding supports, and do not bury a long run in concrete without a movement allowance.
Flush the system before commissioning. Drawing lubricant, brazing flux and cutting debris are the usual causes of pinhole leaks in the first month of service. A clean water flush followed by a pressure test at the specified hold time will reveal most installation defects. Pour l'eau potable, disinfection and a lead-free compliance check are also required in many markets.
En service, monitor water chemistry rather than relying on the alloy name. H68 is comfortable with neutral, low-chloride water. Free chlorine above about 1–2 mg/L, high chloride, low pH or a high dissolved solids level will shorten life. If the water is aggressive, a copper-nickel or a lined tube is the correct upgrade, not a thicker H68 wall.
Idées fausses courantes
- “H68 is the same as H62.” H68 has 67–70% copper and is single-phase; H62 has 60.5–63.5% copper and is stronger but less ductile.
- “All brass tube resists seawater.” Non. H68 is not a marine alloy; seawater causes dezincification and stress-corrosion cracking.
- “Thicker wall always means a better tube.” Thicker wall raises pressure capacity but also raises bending force, poids et coût, and can make expansion difficult.
- “If it bends, it is annealed.” A hard-drawn tube can bend a little and still spring back or crack. Check the temper certificate.
- “Any lead-free solder is fine for potable water.” The filler must be approved for potable water, and the flux residue must be removed.
- “A pressure test is enough.” A hydrostatic test does not find longitudinal seams; eddy-current testing is needed for heat-exchanger tube.
Inspection and Acceptance
Receiving inspection for H68 tube covers grade, dimensions, caractère, surface and test reports. Check OD and wall at both ends and at mid-length, and measure wall at four quadrants to detect eccentricity. Check straightness on a surface plate and ovality with a micrometer or a ring gauge. Look into the bore with a light; a dark ring or a patch of lubricant is a sign that the tube was not cleaned after drawing.
For heat-exchanger tube, require an eddy-current test report and a hydrostatic test report with the test pressure and hold time. Pour l'eau potable, require a lead-content declaration and a flux statement. For brazed assemblies, require a procedure qualification and a sample cut-and-inspect before mass production. A tube that passes dimensional inspection can still fail at the joint if the surface is contaminated or the anneal is wrong.
Foire aux questions
What is H68 brass tube used for?
It is used for condensers, échangeurs de chaleur, radiateurs, water lines, sanitary fittings and decorative tube. It is not intended for seawater or strong chemicals.
Is H68 better than H62 for bending?
Oui. H68 is single-phase and more ductile, so it bends and expands more reliably. H62 is stronger and cheaper but less forgiving.
Can H68 tube be welded?
It can be brazed and soldered. Fusion welding is possible but zinc vaporisation and hot cracking make it difficult; brazing is the normal production method.
What temper should I order for tube-sheet expansion?
Annealed O60 tube with a tight OD tolerance and low eccentric wall. A hard-drawn tube will not expand uniformly and may crack.
Does H68 resist dezincification?
Non. It is more resistant than H62 because of its higher copper content, but it is not a DZR alloy and should not be used in chlorinated or marine water.
How do I check wall eccentricity?
Measure wall thickness at four quadrants at each end. The difference between the maximum and minimum should be within the specified percentage of nominal wall; the thin side governs pressure capacity.
Need H68 brass tube with annealed temper, eddy-current test and export packing?
QIDAMT supplies copper and copper-alloy tube, plaque, strip and bar from Liaocheng. Envoyer une DO, mur, caractère, test requirement and quantity for a quotation.
PROGRÈS