א 7075 aluminium plate is a high-strength aluminium-zinc-magnesium-copper alloy supplied in T6 or T651 temper for aerospace structures, תבניות הזרקה, כלי עבודה, precision machinery and high-load components. It is the strongest common aluminium plate grade, and it is also the least forgiving: it is not weldable, it has poor corrosion resistance without protection, and it moves during machining unless the residual stress has been relieved.

מַה 7075 Plate Is and Where It Is Used

7075 is an Al-Zn-Mg-Cu alloy standardised as AA7075, EN AW-7075 and UNS A97075. The zinc and magnesium additions, combined with copper and a small chromium addition, produce a very high strength after solution treatment and artificial aging. It is not a general fabrication alloy like 6061. It is selected when the part must carry high load with low weight, or when a mold or tool must resist deflection and wear.

Typical uses include aircraft wing and fuselage components, spar caps, landing gear parts, missile and space structures, תבניות הזרקה, לפוצץ תבניות, die-casting tools, ג'יגים ומתקנים, precision machine parts, high-end bicycle frames and components, climbing hardware, robotics and defense equipment. In many of these applications the plate is machined from solid, and the amount of metal removed can be large.

7075 is not recommended for welded structures. The alloy is generally considered non-weldable by arc processes because the zinc-rich grain boundaries can crack during solidification and the heat-affected zone loses strength. If a design requires welding, 6061-T6 or 5083 is usually the better choice. א 7075 part should be bolted, riveted, bonded or machined as one piece.

7075 aluminium plate
A thick 7075 aluminium plate with a mill finish, stacked on a timber pallet and ready for sawing or machining.

ייעוד כיתה והרכב כימי

The certificate should report the alloy, מֶזֶג, heat number and the results of the mechanical tests. The word 7075 אינו מספיק, because T6 and T651 have different residual stress states even when the chemistry is identical. A plate ordered as T6 may machine differently from the same plate ordered as T651, and the difference can be several millimetres of movement on a large part.

אֵלֵמֶנט 7075 לָנוּעַ (%) תַפְקִיד Purchasing check
ו 0.40 מקסימום טוּמאָה High silicon reduces toughness
Fe 0.50 מקסימום טוּמאָה Iron forms coarse phases
Cu 1.20-2.00 Strength and age hardening לְהַלָן 1.2 loses strength
Mn 0.30 מקסימום Impurity and grain control Excess manganese affects quench
Mg 2.10-2.90 Main strengthening element Low magnesium lowers strength
Cr 0.18-0.28 Grain boundary and stress corrosion Too little chromium hurts SCC resistance
Zn 5.10-6.10 Main strengthening element High zinc increases cracking risk
שֶׁל 0.20 מקסימום עידון תבואה Excess titanium affects casting
אחרים 0.05 מקסימום כל אחד, 0.15 max total שאריות Check the certificate

Typical AA7075 / EN AW-7075 window. Confirm the exact standard and temper on the mill certificate.

Zinc and magnesium are the strengthening pair. During solution treatment they dissolve into the aluminium matrix; during aging they precipitate as fine particles that block dislocation movement. Copper adds strength and helps the aging response, while chromium improves resistance to stress corrosion cracking. A heat that is at the low end of the zinc and magnesium ranges may still meet the minimum tensile requirement, but it will have less margin in a highly loaded part.

Iron and silicon are impurities that form coarse intermetallic particles. These particles can act as crack initiation sites, especially in fatigue. א 7075 plate for an aerospace or fatigue-critical part should have iron and silicon at the low end of the range, not merely below the maximum. The certificate gives the numbers; a buyer who only checks the tensile result is missing half the story.

מאפיינים מכניים

7075-T6 is the standard high-strength temper. T651 is the same alloy and temper, but the plate is stretched after quenching to relieve residual stress. The tensile properties are essentially the same; the difference is dimensional stability during machining. For a thin sheet, T6 may be adequate. For a thick plate that will be machined into a large mold or fixture, T651 is usually the correct choice.

נֶכֶס 7075-T6 / T651 typical מַצָב הערת עיצוב
חוזק מתיחה, רמ 572 MPa טמפרטורת החדר Minimum values depend on thickness
חוזק תפוקה, Rp0.2 503 MPa טמפרטורת החדר High strength, low elongation
הַאֲרָכָה, A50 11% טמפרטורת החדר נמוך מ 6061; avoid sharp notches
קַשִׁיוּת אוֹדוֹת 150 חֲצִי פֶּנסיוֹן ברינל Harder than 6061-T6
חוזק גזירה אוֹדוֹת 331 MPa טיפוסי Useful for bolted joints
צְפִיפוּת 2.81 g/cm3 נָקוּב Lightweight compared with steel
מודול אלסטי 71.7 GPa נָקוּב Lower stiffness than steel
מוליכות תרמית אוֹדוֹת 120-130 W/m.K 20 degrees C Heat builds up in dry machining
Solution treatment 465-490 degrees C Mill process Not a shop heat treatment
Aging אוֹדוֹת 120 degrees C for 24 ח Mill process T6 and T651 differ by stress relief

Typical room-temperature values for 7075-T6/T651 plate. Actual minima vary with thickness and standard; use the certificate and the applicable design code.

The combination of high strength and low elongation is what makes 7075 less forgiving than 6061. A sharp internal corner, a deep scratch or a tool mark can become a stress concentration and a crack starter. Design the part with generous fillets, remove tool marks, and do not use 7075 for a part that will be repeatedly bent or hammered. It is a strength alloy, not a toughness alloy.

Thermal conductivity is moderate for aluminium, but the high strength means cutting forces and heat can be significant. In dry machining, heat concentrates at the tool edge and can cause built-up edge or surface cracking. Use sharp tools, positive rake, adequate coolant and a rigid setup. א 7075 part that is machined with a dull tool may pass dimensional inspection and then fail in service because of subsurface damage.

7075 aluminium plate storage
7075 aluminium plates stored on edge in a warehouse, with the thick sections kept separate from thin sheet.

מידות, Tolerances and Plate Data

7075 plate is normally ordered by thickness, רוֹחַב, אורך ומזג. Thickness is the first variable because the strength and the amount of machining stock depend on it. צלחת כלומר 1 mm under nominal may still meet the standard tolerance, but the finished part may be undersize after cleanup. If the design has a minimum finished thickness, add the machining allowance and specify the minimum actual plate thickness.

פָּרָמֶטֶר טווח משותף סובלנות אופיינית What to write on the order
עוֹבִי 6-150 מ"מ ±0.3 to ±1.5 mm נָקוּב, standard and minimum actual
רוֹחַב 1000-2500 מ"מ 0 אֶל +10 מ"מ Finished width after sawing
מֶשֶׁך 2000-6000 מ"מ ±10 מ"מ Cut-to-length or mill length
שְׁטִיחוּת — אוֹדוֹת 3-5 מ"מ למטר Critical for large molds
קִמוּר — אוֹדוֹת 5 מ"מ מעל 3 מ Check before machining
מֶזֶג T6 or T651 לפי תקן T651 for thick machined parts
קָצֶה Sawed or milled Burr and squareness to agree Milled edge for a clean setup
מִשׁטָח גימור מיל No cracks or deep scratches Inspect before machining
Ultrasonic test אופציונלי Per ASTM B594 For aerospace or critical parts

Typical commercial data for 7075 צַלַחַת. Tolerances vary by thickness, width and mill; the purchase order should name the standard and the measured acceptance limits.

Flatness is not a cosmetic requirement for 7075. A plate that is bowed before machining will often distort further when the surface is removed, because the residual stress balance changes. T651 reduces this risk, but it does not eliminate it. If the part is large and thin, plan the machining sequence to remove material from both sides and to support the part evenly. Do not clamp a bowed plate flat and expect it to stay flat after the clamps are released.

Edge condition matters for safety and for machining. A sawed edge can have a burr that cuts gloves or interferes with setup. A milled edge gives a clean reference surface for indicating the part. For a plate that will be machined on both sides, specify a milled edge and a square corner if the setup depends on it. A plate with a ragged edge can slip in the vise and ruin the part.

אֵיך 7075 צלחת עשויה

The process starts with a direct-chill cast ingot. The ingot is homogenised at about 465 אֶל 480 degrees C to dissolve the zinc- and copper-rich phases and reduce segregation. It is then hot rolled to plate thickness, solution treated at about 465 אֶל 490 degrees C, quenched and aged at about 120 degrees C for 24 שעות. The quench must be fast enough to prevent coarse precipitation, but not so fast that the plate cracks.

T651 plate is stretched after quenching, typically by about 1.5 אֶל 3%, to relieve residual stress. The stretch is a controlled permanent elongation that redistributes the internal stress. It is not a straightening operation in the ordinary sense; it is a metallurgical stress relief. A plate that is merely flattened after quenching may look straight but still move when machined.

The most common defects are residual stress, quench cracks, surface scratches, edge cracks, thickness variation and flatness problems. Residual stress shows up as movement during machining, not as a visible defect at delivery. Quench cracks appear at the edges or in thick sections and are a reject. Surface scratches can be removed if they are shallow, but a deep scratch on a high-strength plate can become a fatigue crack starter.

A good mill records the ingot heat number, the solution treatment temperature, the quench delay, the aging cycle and the stretch percentage. The buyer does not need every parameter, but the certificate should connect the plate to a heat number and to the mechanical results. For aerospace or defense work, the traceability requirement is much stricter and may include ultrasonic inspection and a full heat-lot record.

כללי עיבוד וייצור

The first rule is to use T651 for thick machined parts. T6 plate is cheaper and may be adequate for thin parts or parts with symmetrical material removal, but a large mold or fixture machined from T6 can distort by several millimetres. The cost difference is small compared with the cost of scrapping a mold.

The second rule is to plan the machining sequence. Remove material evenly from both sides, keep the part supported, and avoid heavy interrupted cuts that generate heat and vibration. מכונה גסה, stress-relieve if the specification allows, then finish machine. For a large part, a intermediate stress relief can be the difference between a flat mold and a twisted one.

The third rule is tooling. Use sharp, coated carbide tools with positive rake and adequate clearance. Keep the tool path smooth; dwell marks and chatter leave stress concentrations. Use coolant or a minimum-quantity lubrication system that actually reaches the cut. Do not let chips recut; they damage the surface and raise the temperature. א 7075 part that is machined dry with a dull tool may look fine and fail later.

  • Order T651 for thick plates that will be machined on both sides.
  • Allow machining stock on all surfaces; do not design to the nominal plate thickness.
  • מכונה גסה, stress-relieve if permitted, then finish machine.
  • Use sharp tools, positive rake and adequate coolant.
  • הימנע מפינות פנימיות חדות; use generous fillets.
  • אין לרתך 7075; redesign for 6061 אוֹ 5083 if welding is required.
  • Protect the surface from scratches and tool marks before and after machining.
  • Apply a corrosion protection system if the part will be exposed.

Common Mistakes Buyers and Engineers Make

Mistake Why it goes wrong Better practice
Ordering T6 for a large mold Residual stress causes distortion during machining Use T651 for thick machined parts
Trying to weld 7075 Hot cracking and loss of strength Use 6061-T6 or 5083 for welded parts
באמצעות 7075 in a marine environment Poor corrosion resistance without protection לְהִשְׁתַמֵשׁ 5083 אוֹ 6061 עם הגנה
Designing sharp internal corners Stress concentration and fatigue cracks Use generous fillets and smooth transitions
Machining with a dull tool Subsurface damage and heat Use sharp tools and coolant
בהנחה 7075 is tougher than 6061 Lower elongation and notch sensitivity לְהִשְׁתַמֵשׁ 6061 where impact or bending dominates
Ignoring the protective film until late Scratches and contamination Keep the film on until the part is ready
Buying by alloy name only Temper and thickness may be wrong State alloy, מֶזֶג, thickness and standard

Most 7075 failures come from using a high-strength alloy where a tougher or more corrosion-resistant alloy belongs, or from ignoring residual stress.

A frequent engineering mistake is to specify 7075 because it has the highest tensile strength, without checking the fatigue and corrosion requirements. In a cyclic load or a salty environment, a lower-strength alloy with better toughness and corrosion resistance may last longer. Strength is only one design property. The part that survives is the one that matches the failure mode, not the one with the highest data sheet number.

בדיקה וקבלה

Receiving inspection should start with the certificate and the plate label. Check the alloy, מֶזֶג, מספר חום, עוֹבִי, רוחב ואורך. Measure thickness at several points and check flatness on a flat bed. Inspect the surface for scratches, cracks, dents and corrosion. For a thick plate, review the ultrasonic test report if the application is critical.

After machining, inspect the part for distortion, surface finish and dimensional accuracy. A plate that moved during machining may still be within tolerance if the finish pass was light, but the residual stress remains and the part may move again in service. If the part is a mold or a precision fixture, check it after a relaxation period, not only immediately after the last cut.

  • Match the alloy and temper on the label to the certificate.
  • Measure thickness at head, middle and tail, and at three widths.
  • Check flatness and camber before machining.
  • Inspect both faces for scratches, cracks and corrosion.
  • Review the ultrasonic report for thick or critical plate.
  • Record the heat number and plate identity for traceability.
  • Check the finished part after a relaxation period.
  • Keep a sample and the certificate for failure analysis.

שאלות נפוצות

What is the difference between 7075-T6 and T651?

Both have the same alloy and aging treatment. T651 is stretched after quenching to relieve residual stress, which makes it more dimensionally stable during machining. Use T651 for thick machined parts.

פַּחִית 7075 להיות מרותך?

Generally no. Arc welding of 7075 is not recommended because of hot cracking and loss of strength in the heat-affected zone. Use 6061-T6 or 5083 if welding is required.

האם 7075 חזק יותר מ 6061?

כֵּן, considerably. 7075-T6 has about 572 MPa tensile strength versus about 310 MPa for 6061-T6. It is also less ductile and less corrosion resistant.

האם 7075 suitable for marine use?

Not in direct seawater exposure without a protective coating. It has poor corrosion resistance compared with 5083 אוֹ 6061. לְהִשְׁתַמֵשׁ 5083 for marine structures.

למה כן 7075 distort during machining?

Residual stress from quenching and rolling is released as material is removed. T651 reduces the stress, and a balanced machining sequence reduces the movement further.

פַּחִית 7075 be anodised?

כֵּן, but the coating is less uniform and less protective than on 6061. Type II or Type III anodising can be used, and a sealed coating improves corrosion resistance.

What is the maximum service temperature of 7075?

The alloy is not intended for elevated temperature. Strength falls above about 100-150 degrees C, and prolonged exposure above the aging temperature can overage the material.

כמה עולה א 7075 plate weigh?

The density is about 2.81 g/cm3. א 1 m x 1 m plate at 20 מ"מ שוקל בערך 56 ק"ג. Use the actual thickness for freight and handling.

פַּחִית 7075 be used for injection molds?

כֵּן, especially for large molds where high strength and good thermal conductivity are needed. T651 is preferred for thick mold blocks, and the mold should be protected against corrosion.

What is the lead time for 7075 צַלַחַת?

Stock sizes may ship in days; custom thickness, width or ultrasonic testing may take several weeks. Send the full specification for a firm date.

האם 7075 מזון בטוח?

It is not typically used for direct food contact. If it is, the surface finish, coating and applicable food-contact standard must be checked.

Need a 7075 aluminium plate in T651 with a stated thickness and flatness?

בקש הצעת מחיר

אספקה ​​של QIDAMT 7075 aluminium plate from Liaocheng. שלח את העובי, רוֹחַב, מֶשֶׁך, מֶזֶג, flatness and destination for a quotation. Email sales@qidamt.com or call +86 139 6951 8618 during working hours (GMT+8).